search  current discussion  categories  glazes - cone 4-7 

^6 clear for toni in n.m.

updated mon 30 jun 97

 

Robert Speirs, M.D. 766 X4450 on mon 2 jun 97

Toni, here's a really wonderful ^5-6 clear that I use and love. I have
posted it before to Clayart (so you old timers can delete this message
now). It is REALLY clear and shiny, shows no drips, overdips, doesn't
craze and seems not to affect underglazes it covers.

^5-6 Clear

Soda Feldspar 40
Gerstley Bor 30
Ball Clay 20
Flint l0

Hope it solves all your clear glaze problems.

Laura in Oregon