The Allens on sat 20 sep 97
Sorry to be late responding but just now had time to located the recipe:
I love this glaze which I picked up on this group
Sana's Green
potash feldspar 29.12
whiting 9.7
gerst. bor. 11.65
barium carb 7.76 (sub 3/4 strontium - works but color is a little less vibrant)
magnesium carb 2.91
epk 4.85
silica 31.06
tin oxide 2.91
add rutile 4.85
add copper carb 4.85
(I have increased copper carb to 6.00 getting a darker, semi-matt service..don't
| |
|