Cheryl L Litman on mon 9 jun 97
I finally found my book of glaze recipes. Can't remember where I got
this base glaze. Was trading glazes with my sister-in-law in another
state and her studio uses the same one but with a different feldspar.
Base:
29 silica (325 mesh)
5 EPK
20 Kona (sister-in-law uses Custer)
14 talc
32 Gerstley borate
I can't remember what the base alone looks like.
_________________________________________________________
15% red iron oxide - red/brown - looks great under or over the
white
_________________________________________________________
3.5% cobalt carbonate - blue breaking purple
0.5% manganese dioxide
__________________________________________________________
15% zircopax - creamy opaque white (less might work just fine
too?)
__________________________________________________________
| |
|