search  current discussion  categories  glazes - cone 8-10 

^9 "emily purple"

updated tue 30 apr 96

 

Elizabeth Beth Fusaro on mon 1 apr 96


>Jeanne, I also would love your favorite ^9 purple, "Emily Purple" if you
>wouldn't mind sharing.
>
>TIA, DebiBeck

Here's a ^9 "Emily G. Purple" I used to use 15 years ago. Maybe
it is the same one you are looking for. It has a wonderful buttery
texture and is very purple.

Potash Feldspar 410.0
Colemanite 120.0
Dolomite 70.0
Talc 150.0
Tenn. Ball Clay 50.0
Flint (Silica) 200.0
_______
1000.0 gms
Cobalt Oxide 2%
Bentonite 2%
Tin 2%
Beth
Sun & Moon Pottery
Tallahassee, FL