John Post on fri 3 jan 97

Does anyone on the list have an accurate analysis for Alberta Slip that they
could post. I checked at the SDSU web site, but the analysis given there
does not have an LOI listed.

Thanks,

John Post

Bill Amsterlaw on sun 5 jan 97

On 3 Jan 1997 John Post asked:

>>
Does anyone on the list have an accurate analysis for Alberta Slip that they
could post. I checked at the SDSU web site, but the analysis given there does
not have an LOI listed.
<<

Source: Hansen, Tony: "Duplicating Albany Slip" in _The Magic
of Fire_, p.118+ (http://digitalfire.com/index.html)

Alberta Slip #2
---------------
REDEARTH 67.50
WHITING 9.50
TALC 7.00
NEPH SY 14.00
RIO 2.00
100.00


Analysis of Redearth
--------------------
CaO .08 .50%
MgO .26 1.14%
K2O .32 3.29%
Na2O .11 .73%
Fe2O3 .22 3.84%
TiO2 .07 .63%
Al2O3 .55 14.82%
SiO2 3.69 58.47%

L.O.I. 8.40%
RATIO 7.99
WEIGHT 927.74


Anaysis of Albany slip
----------------------
CaO .40 5.86%
MgO .25 2.65%
K2O .13 3.29%
Na2O .11 1.83%
Fe2O3 .11 4.67%
Al2O3 1.34 14.76%
SiO2 10.73 69.41%

L.O.I. 5.70%
RATIO 6.71
WEIGHT 378.93

Analysis of Alberta slip #2
---------------------------
CaO .38 5.92%
MgO .28 3.10%
K2O .11 2.93%
Na2O .11 1.94%
Fe2O3 .11 4.70%
TiO2 .02 .42%
Al2O3 .48 13.67%
SiO2 3.68 61.62%

L.O.I. 5.70
RATIO 7.66
WEIGHT 357.87
EXPAN 6.73


_______________
- Bill Amsterlaw (wamster@msn.com)
Plattsburgh, NY

Tony Hansen on sun 5 jan 97

John Post wrote:
> Does anyone on the list have an accurate analysis for Alberta Slip that they
> could post.

ALBERTA SLIP RECIPE
===================
RECIPE AMT OXIDE FORM ANAL
--------------------------------------------
IXL 45D 27.30 CaO 0.86 7.16
IXL 45R 26.30 K2O 0.24 3.30
M2 10.90 MgO 0.57 3.39
NEPHELINE SYENITE 15.70 Na2O 0.27 2.47
WHITING 10.60 TiO2 0.04 0.45
CYPRUS TALC 7.50 Al2O3 1.00 15.13
BLACK IRON OXIDE 1.40 P2O5 0.01 0.16
IRON OXIDE YELLOW 0.30 SiO2 7.09 63.22
Fe2O3 0.20 4.70
WEIGHT: 674.17 MnO 0.00 0.03
EXPAN: 7.03 L.O.I 9.30
--------------------------------------------

This mix is micropulverized. The black and yellow iron combination were intended
to help match the raw color of Albany. However we have switched to using red or
black according to supplies.

Because Alberta Slip is a blend of materials, we exercise excellent control over
consistency. The clay materials listed are from our quarries. The analysis of
Alberta Slip is calculated from the known analyses of the ingredients.

We are working on a section of our website to take you on a tour of the incredib
quarry sites and give tips of the use of this material.

--
=================================================================
Tony Hansen, Plainsman Clays

Jan Lipuma on sun 5 jan 97

>----------------------------Original message----------------------------
>Does anyone on the list have an accurate analysis for Alberta Slip that they
>could post. I checked at the SDSU web site, but the analysis given there
>does not have an LOI listed.
>
>Thanks,
>
>John Post

John,
Here is analysis from Plainsman Clays for Alberta (Redearth):

CaO .08 .50%
MgO .26 l.14%
K20 .32 3.29%
Na20 .11 .73%
Fe203 .22 3.84%
Ti02 .07 .63%
Al203 1.34 14.76%
Si02 10.73 69.41%

L.O.I. 5.70%

Archie Bray Foundation (406)442-2521 would be able to give you further
info. Hope this helps.

Janice