Susan Goldstein on sun 12 oct 97
Several of you asked for this information.These are formulas that I have
collected from clayart and have not tested so please let me know how they
work for you.
TS Slip (nice orange in soda firing)
Ball Clay 1.5 cups
EPK 1.5 cups
Calgon 2 Tablespoons
Water 20 cups
Shino Slips
#1
Soda Ash 3.2
Spodumene 12.16
Kona F-4 8.64
Nepheline Syenite 36
EPK 28
OM4 Ball Clay 12
Bentonite 3-5% on porcelain
#2
Kona F-4 8
Neph Sy 3l
Spodument 13
Soda Ash 3.5
Helmer Kaolin 35
EPK 10
#3
F-4 18.4
Spodument 15.2
OM-4 Ball Clay 15
Soda Ash 4
Neph Sy 45
EPK 2.4
Bentonite 2
Soda Slips ^11
#1 Copper Slip
Kona F-4 Feldspar 700
Grolleg Kaolin 900
Silica 300
Copper Carb 38
#2 Cobalt Slip
Kona F-4 700
Grolleg Kaolin 900
Silica 300
Copper Carbonate 19
Cobalt Oxide 19
#3 Flashing Slip
Grolleg Kaolin 70
Neph Sy 30
Lithium Carbonate 1
| |
|