Simons, Frank on sun 22 sep 96

Hello Anne, This is a neat brown semi-gloss for cone 6. I beleive it
came from CM, June/81 page 78. It is called Rowe brown
Colmanite 100
EPK 40
Flint 60

Manganese dioxide 10
Red iron oxide 20