Louise Jenks on sat 20 apr 96
Does anyone have a ^6 chartruse oxidation glaze that they would like to
share? ? I use brownish clay so I would need an opaque or semi opaque glaze.
If possible please respond in the next two weeks before I sign off
temporarily for several weeks.
TIA Louise Jenks in Cincinnati
Elizabeth Fusaro on wed 24 apr 96
>----------------------------Original message----------------------------
>Does anyone have a ^6 chartruse oxidation glaze that they would like to
>share? ? I use brownish clay so I would need an opaque or semi opaque glaze.
^5-7 Beth's Shiny Green
Neph. Sy. 43
Titanium Diox. 07
Flint 23
Gerstley Borate 10
Ball Clay 06
Dolomite 10
Bentonite 01
Copper Carb. 1.5%
Hope this works for you. It is between a lime and chartreuse.
Beth Fusaro
Sun & Moon Pottery
Tallahassee, FL
| |
|