search  current discussion  categories  glazes - cone 04-06 

cone 04 to 6 white slip caution

updated thu 31 oct 96

 

Andrew S Lubow on thu 10 oct 96

A short time ago I submitted a ^ 04 - 6 White Slip Base here.

Ball Clay 40%
EPK 20%
Neph Sy 15%
Talc 15%
Flint 10%

Several of my friends have used it with spotty results. While there is no
problem on a body at ^04. At higher cones there can be flaking. Please
test your body when you use this. I apologize for any inconvience this
may have caused but I feel a quick reporting may prevent a bad load.