I am starting a glaze database and am looking for a few glazes to add to
it. If anyone has any blue or deep purple cone 10 reduction glaze
recipies that they would part with i would be most grateful. I am also
looking for (if possible) a matte black (or semi gloss) cone 10 wood fire
glaze. (hopefully to be used as a liner in mugs.

thank you all.
see you at SOFA
Justin

Justin-------->
_| _| _| _| _| _| _| _| _|
_| mujjk8@wiu.edu _|
_| _|
_| School Address _|
_| 115 W. Adams St. Apt. 1 _|
_| Macomb, Illinois _|
_| 61455 _|
_| Phone (309) 833-5428 _|
_| Home Address _|
_| 435 Bode Rd. _|
_| Hoffman Estates, Illinois _|
_| 60194-1622 _|
_| Phone (847) 884-6568 _|
_| _| _| _| _| _| _| _| _|
<--------Kalb

Anne W. Bracker on sat 11 oct 97

The following are a few glazes that I used many years ago! All were used
in a reduction cone 10 gas kiln.

Glenn's Bleu
Custer feldspar 60.0
Whiting 10.0
E.P.K. 5.0
Zinx oxide 5.0
Flint 15.0
Cobalt oxide 1.0
Lite tone rutile 4.0

Add Bentonite 1%

Matt Black
Custer feldspar 40.0
Cornwall Stone 20.0
Whiting 20.0
E.P.K. 20.0
Add
Zinc oxide 7%
Bentonite 2%
Cobalt carb 3.5%
Red iron oxide 1.5%
Mang. dioxide 1.0%

Carron's Blue
Custer feldspar 48.0
Flint 30.0
E.P.K. 2.0
Dolomite 6.0
Zinc oxide 6.0
whiting 10.0
Add
Lite tone rutile 2%
Red iron oxide 3%
Cobalt oxide .5%

Celadon Zircopax (we called it "Hospital White") - Nice with Rand's bleu)
Custer feldspar 41.2
Whiting 14.8
Magnesium Carb 2.5
Zinc oxide 3.6
E.P.K. 3.8
Flint 34.1
Add
Zircopax 10%
Bentonite 1%
(I believe the original glaze was out of either the Nelson or Rhodes book
& that I altered it.)
Anne

Bracker Ceramics
1835 E 1450 Road
Lawrence, KS 66044

1 913 841-4750 OFFICE
1 913 841-8142 FAX
1 888 822-1982 ORDER LINE
bracker@midusa.net E-MAIL

"Clay Ain't Dirt"