Darlene Yarnetsky on fri 31 may 96

Sue-

Here's a peach I've developed; maybe it will give you a starting point.
Be sure to try it at different thicknesses. I've fired it from cone 5-8
with best results at a high cone 6 or low 7. Can get runny at 7 if
applied too thick. Good luck!

Cone 6 Lt. Peach:

Gerstly Borate 46
EPK 16
Flint 38

Add -- 10% powdered rutile


Darlene Yarnetsky -- Mudcat Pottery
Madison IN