search  current discussion  categories  glazes - cone 4-7 

cone 6 textures addendum

updated thu 31 oct 96

 

"Rafael Molina-Rodriguez (Rafael Molina-Rodriguez)" on fri 18 oct 96

Clayarters:

Here are three more cone 6 (Cone 7 in sitter) oxidation textured wood
ash and fake ash glazes from Ceramicsweb/gopher :

Fake Ash

Whiting 20
Ferro Frit 3134 20
Custer Feldspar 20
Barium Carb 15
EPK 15
Gerstley Borate 10
100

Nickel Oxide 5


Zakin's GK Ash

Ferro Frit 18.18
Magnesium Carb 7.07
Neph Sy 10.10
Strontium Carb 11.11
Spodumene 15.15
EPK 10.10
Whiting 13.13
Wood Ash 15.15
100.00

Opax 12.12
Bentonite 2.02


Ash Glaze

Gerstley Borate 13.60
Lithium Carbonate 4.50
Wood Ash 18.20
Whiting 18.20
Albany Slip 36.40
Kaolin 9.10
100.00

Very nice textures, but still not quite like high-fire reduction glazes.