Sandra Dwiggins on fri 13 jun 97
Hi Clay people (always makes me think of Flash Gordon)---
Here is the Deep Purple Glaze I teased you with. I have seen the error
of my ways and I'll ALWAYS give the formula with the description hence
forward...
The glaze was submitted by Jan Walker and tested first by her...
Deep Purple ^6 Ox (^7 in sitter)
Gerstley Borate 8.4
Neph Sy 14
Pot Spar 27
Whiting 12
Lith Carb 3.7
Magnes Carb 1.7
Flint 33
Bentonite 2
Cob Carb 0.6
Chrome Ox 0.17
Enjoy!
Sandy
Emily Muench on tue 1 jul 97
Hello Sandy and all
I tried the deep purple glaze this weekend, and though the result was a
very beautiful satin-matt blue it wasn't purple. Did anyone have the same
experience?What did I do wrong? I'd love to have a purple ^6 glaze!!!!!
Thanks for your help.
Sandra Dwiggins on wed 2 jul 97
If it was satin matt, it could have been slightly underfired.
| |
|