search  current discussion  categories  glazes - misc 

foaming glaze

updated fri 26 jan 01

 

Jonathan Kaplan on sun 12 may 96

One of the easiest ways to decrease or eliminate excessive foaming
in glazes is to add a small amount of defoamer, available from swimming
pool or spaw maintenance companies.

Jonathan


Jonathan Kaplan
http://www.craftweb.com/org/jkaplan/cdg.shtml


(aka "Scooter)
jonathan@csn.net
Ceramic Design Group Ltd./Production Services Voice:
970-879-9139 POB 775112
FAXmodem: same
Steamboat Springs, Colorado 80477, USA CALL before faxing



"No matter where you go, there you are!"

Puddy & Co. on wed 24 jan 01


Cindy,
what do you mean by "foaming"? Is it bubbles that run on the surface of
the glaze in the bucket as you move it or shake it , sort of "coca
cola" type of bubbling? I had this problem with a glaze containing
spodumene. At Ron Roy's advice I wash my spodumene before mixing it into
the glaze - measure it, soak it in water, let it settle, pour the water
off, do it 6 times. The foamy scum comes out really nice and the glaze
is usable again. Works.

Happy washing

Hanna Lewandowski
Auburn, Ontario