P. Jaine Jacobs on wed 4 dec 96
In a message dated 12/4/96 1:08:56 PM, you wrote:
>(In particular, lately I've wanted to use
>a reliable cone 10 black satin/waxy glaze, in case you know of one.)
Eric, you might like to try Charlie D Manganese. I've seen it used
successfully at the 92nd Street Y in the gas kiln, cone 10, reduction for
more years than it would be discreet to say:
20% Custer spar
20% Kona F4
2% Whiting
15% Dolomite
13% Talc
10% Ball Clay
20% Flint
=100% total;
then add 2% Bentonite and 4% Manganese
Hope you enjoy it,
Jaine in Cresskill
| |
|