glaze recipes for ^10 in oxidation

updated sat 30 nov 96

 

sutter on mon 28 oct 96

Good morning all!
I'm looking for a few good recipes to try out. I really would love a
satiny cream kind of off white, and maybe something in a turquoise. I
use a Bmix and Colemans Porcelain. Thank you for all the help.

Debra Sutter
Go North Pottery
Anchorage, AK.... the days are getting shorter, the world is still white
from my window as I type this, more snow expected tomorrow.
Have a nice day!

LizzardOL@aol.com on fri 1 nov 96

We typically fire our cone 10's in reduction because we don't have an
electric kiln that fires that high. Still, these recipies ought to work in
reduction - at least worth a try:

Waxy White Matt

Custer Spar 41
Gerstley 14
Dolomite 7
Kaolin 5
Flint 21
Ultrox 6

For turquoise add: 1% cobalt carbonate & 1% Chromium Oxide

Yields a nice matt turquoise.

Liz Dodge
Berkeley., CA

LizzardOL@aol.com on mon 4 nov 96

We typically fire our cone 10's in reduction because we don't have an
electric kiln that fires that high. Still, these recipies ought to work in
reduction - at least worth a try:

Waxy White Matt


WHOOPS - I meant to say this recipe ought to work in OXIDATION.