search  current discussion  categories  glazes - misc 

glaze recipes, please

updated sat 31 aug 96

 

Marty McFarland on wed 21 aug 96

I am looking for a recipe or formula for a purple glaze, a pink glaze
and a red glaze, all for cone 6 glazing.

Any help any of you can give would be greatly appreciated.

KEMPB on fri 23 aug 96

In answer to your request for purple, pink and red glazes for Cone 6. Try
these

Pink
Gerstley Borate 21, Nepheline Syenite 16, Kaoling 11, Whiting 20, Silica
32, Tun Oxide 5, Chromium Oxide 0.15.
Purple
Potash Feldspar 37, Gerstley Borate 12, Dolomite 6, Talc 14, Kaolin 5,
Slica 23, Zinc Oxide 3, Cobalt Carbonate 2
Tomato Red
Nepheline Syenite 55, Silica 25, Kaolin 10, Dolomite 10, Bone Ash 10,
Red Iron Oxide 10, Bentonite 2

Brian Kemp. Singapore