search  current discussion  categories  glazes - misc 

glazebase reaches 20

updated mon 31 mar 97

 

Robert Wilt on thu 13 mar 97

------------------
This week the GlazeBase project received the 20th submission
of the year, so I'd like to give you a brief summary of the glazes
and publicly thank those who have taken the time to submit them.

The full glaze recipes and notes can be viewed from the
GlazeBase page:
http://www.tiac.net/users/rjw/gbpage.htm
That is also where you can find the form to send in your own
contributions.


=2A=2A=2A From Rick Malmgren (RMalmgren=40juno.com), whose favorite
Ice Cream Flavor is Bryer's Mint Chocolate Chip:

Emily's Purple c/6-8 Ox./Red. Semi-gloss Blue to purple

=2A=2A=2A From Richard Burkett (richard.burkett=40sdsu.edu), whose favorite
Ice Cream Flavors are Ben and Jerry's Pistachio and Cranberry Orange
sorbet:

Midrange Majolica 96 c/5-7 Oxidation Gloss white majolica base
Meloy Clear revised c/8-10 Reduction Gloss very clear

=2A=2A=2A From Suzanne (SuzZim=40swbell.com), who apparently prefers to =
remain
neutral about ice cream flavors:

Copper Red (U. Houston) c/9-11 Reduction Gloss oxblood red

=2A=2A=2A From Sam Cuttell - alias the cat lady (scuttell=40wwdc.com) who
prefers Mowie Cowie:

Oxidation Temoku c/10 Oxidation Gloss black breaking to brown

=2A=2A=2A From bob kavanagh (bkav=40vax2.concordia.ca), who likes black =
cherry
ice cream:

bob's base c/6-9 Oxidation Gloss slightly grey

=2A=2A=2A From Peggy Heer / Heer Pottery (p4337=40connect.ab.ca) who prefers
Chocolate ice cream:

Transparent/Clear c/9-10 Ox./Red. Gloss Clear

=2A=2A=2A And finally, from Edouard 'Bass' Bastarache
(edouardb=40sorel-tracy.qc.ca), whose favorite ice cream flavor is
generally Vanilla but at this time of year likes Maple Polkadot
Vanilla:

Bass Bleu c/8-10 Reduction Gloss Deep blue
Mag. 8-10 Reduction Semi-gloss Light tan
Benji's ash glaze 8-10 Reduction Satin matt Tan
Felix's Green Ash Glaze 8-10 Reduction Waxy Green
Blanc Julien Glac=E9 8-10 Reduction Gloss White
Blanc de Michel 8-10 Reduction Semi-gloss Satin white
Vert jade cendr=E9 04 Oxidation Semi-gloss Jade green with =
texture
Blanc cendr=E9 8-10 Reduction Gloss Cream white
Noir Lindo 8-10 Reduction Gloss Black
Bleu textur=E9 8-10 Reduction Semi-gloss Blue textured
Vert antique 8-10 Reduction Semi-gloss Medium green
Feuilles d'automne 8-10 Reduction Semi-gloss Yellow-green and red
Bleu Ginette 04 Oxidation Gloss Dark blue, white =
mottling

Many of Edouard's glazes are original glazes invented by him and his
friends. Several are ash glazes.

That's it for now=21

waiting for the next 980,