R Wuetherick on thu 24 oct 96

> From: Sue Davis
> ----------------------------Original message----------------------------
> This Honey Glaze looks good but I fire in the ^6 range. Can you adjust
this
> one for me to try at that cone? Thanks.

I haven't tested this but give it a try and let me know! I have been
reformulating glazes for a short
time. Maybe some of the glaze guru's out there could make a comment about
this. Therby helping
you find a glaze and I in learning...

Good Luck!

9642 Weisers Honey (C6)
=======================
POTASH FELDSPAR. 20.00 20.00%
GERSTLEY BORATE. 20.00 20.00%
NEPHELINE SYENIT 20.00 20.00%
FLINT........... 15.00 15.00%
WOLLASTONITE.... 10.00 10.00%
DOLOMITE........ 2.00 2.00%
EPK KAOLIN...... 5.00 5.00%
IRON OXIDE RED.. 7.00 7.00%
TITANIUM DIOXIDE 1.00 1.00%
==========
100.00
FORMULA & ANALYSIS
==================
*CaO .49 9.53%
*MgO .04 .50%
*K2O .14 4.61%
*Na2O .19 4.09%
*Fe2O3 .14 7.47%
TiO2 .04 1.08%
P2O5 .00 .01%
B2O3 .46 11.11%
Al2O3 .31 10.96%
SiO2 2.46 50.64%

COST/KG 1.08
RATIO 7.85
EXPAN 8.43
WEIGHT 290.91