Here ar two majolica glazes you can try
Arbuckle Majolica cone 03
frit 3124 65.75
F-4 feldspar 17.24
EPK 10.82
neph sy 6.24
tin 5
zircopax 10
bentonite 2
1/2 -3 tbsp Epsom salts to 5 gallons of glaze


Anderson Majolica cone 04
frit 3124 55
ball clay 10
flint 10
zircopax 8

Hope one of these is what you are looking for.
Posey