RUST RED ^6

Flint 30.46
Gersley Borate 30.18
F4 20.20
Talc 14.18
EPK 4.98
------------------------------
total
also add
Red Iron Oxide 18.10
Bentonite 3.00



It is a glossy red/greyish pale green fused together. It is very nice.