Lari Ward on tue 20 may 97
The following glaze was tested and was supposed to be a nice translucent
cobalt glaze at 04. What I got was a speckly transparent clear/cobalt
glaze. The cobalt produced speckles rather than being "homogenized". Can
anyone fix this glaze or do you have one that works?
Frit 3110 75%
Grolleg 15
Flint 10 Thanks! How do you make smiley faces on
a computer?
Cobalt 1.5 Lari in Poulsbo, Wa
Zirconium 5
Tony Hansen on wed 21 may 97
Lari Ward wrote:
> The cobalt produced speckles rather than being "homogenized". Can
> anyone fix this glaze or do you have one that works?
Use a blue stain or cobalt carbonate instead of cobalt oxide.
Mason 6300 is good.
--
=================================================================
Tony Hansen, IMC thansen@mlc.awinc.com
| |
|