Axner on wed 3 apr 96
Dear Eveline,
Laguna Clay has a very nice earthenware clay body. It's called "Red
Earthenware EM207". It is a very nice throwing body. There is no grog or
sand in this clay.
The following cone 04-03 glaze will work well with it.
Frit 3124 65.75%
F-4 Feldspar 17.24
Kaolin 10.82
Nepheline syenite 6.24
Tin 5.00
Zircopax 10.00
Bentonite 2.00
Give it a try and I hope it works for you.