Sana's Green (original formula)
============
Ingredient Amt (g) Amt (%)
---------- ------- -------
Potash Feldspar 1200 29.12
Whiting 400 9.70
Colemanite 480 11.65
Barium Carb. 320 7.76
Magnesium Carb. 120 2.91
EPK 200 4.85
Silica 1280 31.06
Tin Oxide 120 2.91
---- ------
4120 99.96

Copper Carb. 200 4.85
Rutile 200 4.85
Bentonite 82 2.00