search  current discussion  categories  glazes - cone 8-10 

pink shino glaze cone 9-10

updated fri 28 feb 97

 

Leon Popik on fri 21 feb 97

I recall seeing someone wanting a pink glaze, but I cant remember who
needed it . Here is the recipe for a Pink Shino glaze we used in school.


Pink Shino (cone 9-10)

14.6 Kona Spar
12.5 Spodumene
3.0 EPK
3.0 Soda Ash
50.0 Neph. Sy
16.5 Ball Clay (OM4)
6% Mason Alumina Pink stain

Looks Hideous inside mugs, but would have great possibilities in Soda or
Wood firings.