Here are a few very reliable raku glaze recipes:
Crackle White
Gerstley Borate....70%
Neph Sy....30%
Matte Copper
Red Cupric (Copper) Oxide....78.26%
Red Iron Oxide....8.70%
Ferro Frit 3110....13.04
Racoon Copper (shiny) - recipe for 1110 gm batch
Kingman (potash) feldspar...120
Gerstley borate....630
Flint (silica)....120 (like, 200 mesh)
Ball clay....60
Barium carbonate....60
Copper carbonate....120
Enjoy...Best regards, Ellen Baker - Glacier, WA