Jaine & George on fri 27 dec 96
To all of you, a happy and healthy new year, and especially for Gary,
Louise, and everyone else who asked, some raku recipes:
* Del Favero Lustre *
4000 Gerstley Borate
1000 Cornwall Stone
100 Copper Carb
* Soldner Red *
200 Colemanite or Gerstley Borate
200 Borax
40 Copper
40 Rutile
* Alkaline Blue *
700 Frit 3110
50 Colemanite or Gerstley Borate
100 Flint
100 Soda Ash - well ground
50 EPK
30 Copper Carb
* White (well clear, actually) Crackle *
65 Gerstley Borate
20 Neph Sy
5 EPK
10 Flint
* Copper Matte *
10 Frit 3110
90 Copper Carb
* Great Metalic Red *
63 Gerstley Borate
12 Custer Spar
12 Flint
6 Ball Clay Om #4
6 Barium (oh, no) carb
then add 12% Copper Carb
Enjoy,
Jaine in Cresskill
| |
|