LINDA BLOSSOM on sat 3 may 97

Hi Marshall,

I was going through printouts and found the one where you asked me for red
recipes. I can see it doesn't work to leave them in the inbox and it
doesn't work to print them out. I had a stack of filing that rivaled
anything the government could have created. Anyway here are three recipes.
The first firedup as a soft red and the other was ruby red. However, that
was just in one firing. In the next firing for each one, a new glaze
emerged. I've been firing oxidation to clear my head for a while.

whiting 10.42
MgCO3 1.04
custer 57.29
siica 31.25
tin 2.13
CuCO3 1.04



custer 59.8
3110 11.3
zinc oxide 5.15
talc 4.1
whiting 16.5
epk 3.1
CuCO3 1
tin 2



Linda Blossom
2366 Slaterville Rd.
Ithaca, NY 14850
607-539-7912
blossom@lightlink.com
http://www.artscape.com