MARK BELL LICHEN - CONE 6-8
Soda Spar 30
Magnesium Carbonate 31
Frit 25 (3269) 6
Talc 8
Zinc Oxide 6
Kaolin (tile 6) 19

I got this glaze from Lana Wilson's info from an NCECA so years ago.