Don Goodrich on wed 21 aug 96
Valice,
From my old college notebook, here's a ^08 luster raku glaze I've used a
couple of times. Used it as a reflective surface in the back of a wall
sconce. After seven years and some polishing it still has a mirror-like
luster (although in some spots more gold than silver).
Gerstley borate 80
Cornwall stone 20
Silver chloride 5
The notebook also says "reduce in straw, should be fumed". Good luck!
--Don Goodrich in Zion, Illinois
| |
|