Cindy P Russell on thu 18 apr 96


This to all of those that requested the clear glaze that I talked about a
few days ago.

Simple Clear Glaze

Gerstly Borate 44.64
EPK 26.79
Flint 28.5

Hope this works for ya'll. It has worked on a variety of clays for me
and I have used it over underglazes. It is a cone 6 oxidation glaze.


Cindy Russell