Lori Wilkinson on sat 6 apr 96

Hi all,

First of all I want to thank everyone for their help with the Black glaze
receipes. Here are the results and also the results from some from the
database with very minor changes all on Dillo White at a full ^6.

Reeds Glory Black
Gerstley 11
EPK 5
Custer feldspar 79
Whiting 5
Add:
Copper Carb 4
Mang. Dioxide 6
Coblat ox 2
RIO 1
A true glossy black

Mirror Black
Custer Feldspar 42
Zinc ox 12
EPK Kaolin 15
silica 26
Whiting 15 yes, I know this does not equal 100%
Add
RIO 8
Cobalt Carb 2
A true glossy mirror black

Black With Gold Candice, check
this out for your baskets
Kentucky Ball Clay 3.9
C.H. Redart Clay 47.8
Flint 3.9
Copper Carb 4.9
Cobalt Carb 3.9
Mang. dioxide 35.6
~~~~~~~~~
100% Dull satin black with a
bronz cast

^6 Ash Glaze
Red Art 40
Frit 3124 30
Ash 30 I used sieved unwashed
fireplace ash
Rutile 4
An excellent honey gold gloss

Add 3% cobalt for a perfect Black

Fake Ash

Gerstley 50
Barnard Clay 25
EPK 25

Nice light glossy golden brown but not really a runny glaze

Ten ZA

Custer Feldspar 43.20
EPK 9.88
Silica 23.46
Whiting 11.11
Gerstley 12.35

Add
RIO 9.88
Glossy light Honey Gold, much like a fake ash

Soft Green With Pink Flecks

Neph Sy. 67
Dolomite 10
EPK 8
Silica 9
Zinc Ox 6

Add
Copper Carb 3

Exquisite light green gloss but no pink flecks

From the database I also tried out an "army green" that turned out a mat
royal blue and a "Strong Pink" that turned a very crawling blah celery green.

Thanks again. You all are really great.

Lori Wilkinson in Roswell NM Where we got some precipitation today for the
first time since last
fall - - an entire 2/10 of an inch of rain and it took all day
to fall.

RidgeviewS@aol.com on mon 8 apr 96

Hi all... I am very interested in glaze recipes being shared online... also,
it would be of interest to me to also know whether results of tests were done
in an oxidation or a reduction atmosphere.

Thanks for sharing all of the great sounding glazes... can't wait to test
them!
JMThom
Boulder, CO