turquoise matt glaze cone 5?

updated sat 31 aug 96

 

John Baisch on wed 31 jul 96


Hello All

I'm looking for a recipe for a turquoise matt glaze, cone 5.

If anyone has any suggestions they would be greatly appreciated...


JB
In Boise, where hot has a new meaning

~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~
~~~~~~ John Baisch ~~~~~~~~~~~~~~~~~~~~~~~~
~~~~~~~~ E-Mail: jbaisch@micron.net ~~~~~~
~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~

Kathy Schuetz on tue 6 aug 96

John Baisch asked for a turquoise matt ^5 glaze for oxidation. Here is a recipe
from the Potters Guild of Baltimore.

Turquoise Matt ^5 Oxid.

Strontium 120 grams
Neph Sy 280
EPK 18
Flint 32
Lithium Carb 8
Copper Carb 20
Bentonite 8

Kathy Schuetz