Art Powell on mon 14 apr 97
Dan,
Here's a white glaze which may meet your requirements. My wife
went to a funeral in Saskatoon, wandered into a pottery store and
came home with this recipe on the understanding we pass it on. I
have been using it quite successfully.
Lindberg white
Flint 29
Calcium carbonate 13
Frist 3134 19
Kona F4 20
Kaolin - pioneer 19
Superpax 12.5
Art Powell
Black Bear Pottery,
Kitamaat Village, B.C.
e-mail: apowell@yellowhead16.net
Robert Acton on tue 15 apr 97
Could you please post what cone the glaze is for.
Dan Saultman on wed 16 apr 97
Robert Acton wrote:
>
> ----------------------------Original message----------------------------
>
> Could you please post what cone the glaze is for.
Robert, I was the original poster of the question for a white paint
like glaze. I received several really great recipes. In a week or so
I'll post the results for you and others on the network. Pretty windy
way of geting around to answering: CONE 6.:)
Dan Saultman on the edge of the mountains in Colorado.
| |
|