Alisa Clausen on wed 2 may 07


Glaze test for Honey Green,. Cone 6, Ox.

Source: Don Goodrich

Credited to:

Fired on mid fire white stoneware

Firing ramp with an electric controller is:
100c p/h to 600c (212f - 1112f)
150c p/h to 1140c (302f - 2084f)
80c p/h to 1220c (176f - 2228f)
15 min. soak
cool down max. to 900c (1652f)
Hold 30 minutes
Shut off kiln


Recipe Name: Honey Green, Don Goodrich

Amount Ingredient
20 Frit--Ferro 3124
20 Nepheline Syenite
20 Feldspar--Custer
15 Flint
10 Wollastonite
2 Dolomite
5 Kaolin--EPK

92 Total

Additives
3 Iron Oxide--Red
1 Titanium Dioxide
.5 Cobalt Oxide
3 Copper Carbonate

Unity Oxide
.241 Na2O
.127 K2O
.057 MgO
.575 CaO
1.000 Total

.461 Al2O3
.153 B2O3
.003 Fe2O3

3.783 SiO2
.001 TiO2
0 P2O5

8.2 Ratio
7.5 Exp

Comments:
Gloss, transluscent, honey brown glaze. Green cast where thickest.