search  current discussion  categories  glazes - misc 

glaze test for shiny clear gtb-1

updated thu 3 may 07

 

Alisa Clausen on wed 2 may 07


Glaze test for Shiny Clear GTB-1
Source: Ceramic Arts Buyers Guide, 2007

Credited to: Wayne Bates, to use over his engobes.

Fired on mid fire white stoneware

Firing ramp with an electric controller is:
100c p/h to 600c (212f - 1112f)
150c p/h to 1140c (302f - 2084f)
80c p/h to 1220c (176f - 2228f)
15 min. soak
cool down max. to 900c (1652f)
Hold 30 minutes

Shut off kiln

Colorants or additives to a 100 gram batch are measured in percent to the
100 gram batch.

Substitutions in this test: Frit 3134 subbed with local Boron Frit,
Feldspar used is Forshammer, Boron Frit is subbed for Gerstley Borate. All
substitutions are done not by Mol. Wts., but gram for gram.
Amount Ingredient
8 Whiting
27 Gerstley Borate--1999
39 Nepheline Syenite
8 Kaolin--EPK
18 Silica

100 Total


Unity Oxide
.275 Na2O
.072 K2O
.006 MgO
.647 CaO
1.000 Total

.508 Al2O3
.369 B2O3
.002 Fe2O3

3.148 SiO2
.001 TiO2
0 P2O5

6.2 Ratio
7.6 Exp
Results
Gloss, transluscent glaze. Badly crazed on my claybody.

Best regards, Alisa from Denmark