another proposition
Frit 3134 42
Silica 12
Redart clay 46
Na2O 0.28 Al2O3 0.30 SiO2 3.99
K2O 0.07 B2O3 0.54 P2O5 0.00
MgO 0.06 TiO2 0.02
CaO 0.59 Fe2O3 0.07
Alumina:Silica ratio is 1.00:13.42
Neutral:Acid ratio is 1.00:4.85
Alk:Neut:Acid ratio is 1.00:0.84:4.08
Expansion: 71.1 x 10e-7 per degree C
Oxides causing abnormal expansion:
B2O3