Tom at Hutchtel.net on mon 10 sep 07
Chris....are you sure nothing's missing? Adds up to 59.
Tom Wirt
From: "Chris Rose"
Sent: Monday, September 10, 2007 8:51 AM
Subject: Found: Sea Foam Zinc
found the ^10
> Sea Foam Zinc recipe I had misplaced. I cannot attribute the glaze other
> to say that I didn't originate it. Here is what I found;
>
> Sea Foam Zinc ^10 ox or redux
>
> Dolomite 12.0
> Zinc Oxide 6.0
> Whiting 8.0
> Neph Sy 37.0
> EPK 2.0
> Copper Carb 2.0
> Rutile 5.0
>
Tom at Hutchtel.net on mon 10 sep 07
Second shot...I would guess it's silica? that's missing?
Tom
Chris Rose on mon 10 sep 07
All,
Just to close on my question from the other day, I finally found the ^10
Sea Foam Zinc recipe I had misplaced. I cannot attribute the glaze other
to say that I didn't originate it. Here is what I found;
Sea Foam Zinc ^10 ox or redux
Dolomite 12.0
Zinc Oxide 6.0
Whiting 8.0
Neph Sy 37.0
EPK 2.0
Copper Carb 2.0
Rutile 5.0
A glossy light green (minty maybe) with some action due to the rutile.
Breaks clear over edges.
Best,
Chris
| |
|