search  current discussion  categories  glazes - traditional iron glazes 

shaner shino slip

updated wed 13 feb 08

 

Bill Merrill on mon 11 feb 08


Soda Ash 3 60

Spodumene 13 260

Kona F-4 8 160

Neph Sy 36 720

EPK 28 560

Ball Clay 12 240

100 grms 2000 gms.

=20

This is a "Shaner" slip. The ball clay can be replaced with another
flashing clay like Helmer. The Epk and OM4 add up 40% of the slip. The
clay content will determine how you will apply the slip, to leather hard
ware, to bisque ware or green ware. =20

David Shaner's Shino-type slip glaze

Neph. Sye=20

36

Koalin=20

28

Spodumene=20

12.2

OM4 Ball clay=20

12

Soda ash=20

3

=20

=20