Recipe Name: Rhodes Turquoise ^6 ox.

Cone: 6 Color:
Firing: Oxidation Surface: Glossy

Amount Ingredient
0
0
0

0 Total


Unity Oxide



0 Ratio
0 Exp

Comments: Glossy glaze with a dark green ground. Surface has a shell of
turquoise and blue variegation. Green turquoise where pools.





















-----------------------------------
Calculations by GlazeMaster=99
www.masteringglazes.com
------------------------------------

Alisa Clausen on thu 28 feb 08


Recipe Name: Rhodes Turquoise ^6 ox.

Cone: 6 Color:
Firing: Oxidation Surface: Glossy

Amount Ingredient
45.5 Feldspar--Kona F4
8.3 Whiting
4 Zinc Oxide
6 Dolomite
13.7 G.B. subbed with Frit--Ferro 3134
20 Silica
2.5 Kaolin--EPK
3 Bentonite

103 Total

Additives
2 Cobalt Carbonate
4 Copper Carbonate
2 Superpax
2 Rutile

Unity Oxide
.208 Na2O
.065 K2O
.093 MgO
.497 CaO
.137 ZnO
1.000 Total

.287 Al2O3
.126 B2O3
.003 Fe2O3

2.763 SiO2
0 TiO2
0 P2O5

9.6 Ratio
7.6 Exp

Comments: Glossy glaze with a dark green ground. Surface has a shell of
turquoise and blue variegation. Green turquoise where pools.




























-----------------------------------
Calculations by GlazeMaster=99
www.masteringglazes.com
------------------------------------