The info. for Clear ^6 is not accurate. It should read:


Recipe Name: Clear ^6
Cone: 6 Color:
Firing: Surface: Glossy
Amount Ingredient
51 Nepheline Syenite
22 Gerstley Borate--1999
14 Wollastonite
8 Kaolin--EPK
3 Zinc Oxide
2 Titanium Dioxide
100 Total



Unity Oxide
.265 Na2O
.073 K2O
.019 MgO
.537 CaO
.106 ZnO
1.000 Total
.473 Al2O3
.235 B2O3
.003 Fe2O3
2.24 SiO2
.073 TiO2
0 P2O5
4.7 Ratio
8.6 Exp
Comments: gloss, transluscent, crazed
used Frit, higher Alum.





-----------------------------------
Calculations by GlazeMaster=99