search  current discussion  categories  glazes - cone 04-06 

low fire bark glaze

updated tue 18 nov 97

 

Beverly Crist on mon 17 nov 97

Here's a glaze that I used on a piece that I wanted to look like a tree
stump. It comes out rough textured and a mottled green and chocolate brown.
I brushed it on thick.

Bob Shay's Lichens, cone 04, electric

magnesium carb. 50
lithium carb. 10
borax 50
gerstley borate 30
copper carb. 4
cobalt carb. 0.4


Beverly Crist, Dallas, Texas
atcrist@aol.com