search  current discussion  categories  glazes - cone 8-10 

cone 10 grey semi-matte

updated wed 2 apr 08

 

Dan Saultman on tue 1 apr 08


Hello all,

Does anyone have a reliable cone 10 redux grey glaze they would share
with me please?
I use a white clay body.


Thank you.


Dan Saultman
Fine-Art Pottery
Detroit
http://www.saultman.com

Nobody Special on tue 1 apr 08


On Tue, 1 Apr 2008 18:48:38 -0500, Dan Saultman wrote:

>Hello all,
>
>Does anyone have a reliable cone 10 redux grey glaze they would share
>with me please?
>I use a white clay body.
>
>
>Thank you.
>
>
>Dan Saultman
>Fine-Art Pottery
>Detroit
>http://www.saultman.com
>
>______________________________________________________________________________
>
Dan...

Here is a never-fail warm soft grey semi-matte that I used extensively. It
is a studio glaze from Adrian College, in scenic Adrian, Michigan:

Shepard Road Ash, cone 10:

Unwashed hardwood ash 40
Custer Spar 40
OM4 Ball Clay 20

That's it. No colorants, no nothing. Don't let the "ash" part fool you;
this is not a typical ash rivulet glaze. It is stiff and opaque, a really
nice and trouble-free glaze.

Hope it works for you. As always, YMMV.

...James