Richard Aerni on mon 9 jun 08
Gang:
Here are glazes that appeared on the bowl in question from earlier this
week:
Ted's White Cone 9-10 O or R
This one I've obviously had around for a long time...the index card in my
filebox is from the late 70s
Soda Spar 63 (Steve Slatin had an interesting thought about soda and
titania blues)
OM 4 Ball Clay 10
Silica 7
Whiting 5
Dolomite 15
100%
Rutile 7
Tin Oxide 7
Bentonite 4.5 (for single fire purposes)
Aerni Crystal Matte (I'm including a couple of recipes...not sure which I
used on the piece)
Custer Spar 44
Strontium 10
Whiting 18
EPK 18
Frit 3124 5
Lithium Carb 5
100%
Titanium Dioxide 15
Bentonite 4.5
Tom Coleman/Steven Hill Crystal Matte (?)
Custer Spar 40
Whiting 15
Strontium 11
#6 Tile Clay 12
Frit 3124 4
Lithium Carb 4
Zinc Oxide .5
Titanium Dioxide 15
101.5
Bentonite 4
Yet Another Anonymous Crystal Matte Glaze
Custer Spar 50.0
Whiting 8.9
Zinc Oxide 8.9
Barium Carb 21.0
OM 4 10
Lithium Carb 2.0
Rutile 2.0
102.8
Bentonite 4.5
Tom Coleman Spotted Black
Whiting 6.12
Custer Spar 79.6
Silica 14.28
100%
Yellow Iron Oxide 20.41
Bentonite 4.5
Neu Sheffield Rim/Base glaze
Sheffield Slip Clay 60
Frit 3134 20
Whiting 10
Neph Syenite 10
100%
Bentonite 4.5
Chrome Oxide 1
Red Iron Oxide 2
Manganese Diox 2
Cobalt Carb 2
And I think I listed the wood ash glaze recipes in the earlier post.
That's all folks! Good luck to those who want to try it...
Richard
Richard Aerni
http://www.richardaerni.com