Chic Lotz + keith Montgomery on tue 10 jun 08
Have been looking for that ^6 Electric Shino recipe that combines a
White Satin and Nutmeg. I remember it was discussed quite a bit a
few years ago. Tried searching the archives, but it says I am not
authorized to do so. If you have the two recipes for mixing this
glaze, can you email them to me off line. I'd also like to know the
author of that glaze if possible......
Thanks, Chic Lotz
Chic@PotteryPoet.com
www.PotteryPoet.com
Kim Hohlmayer on wed 11 jun 08
Hi All,
That ^6 Shino sounds yummy. If someone comes up with those two recipes, don't just email them to Chick and Keith, Share, please. Thank you!!! --Kim H.
--- On Tue, 6/10/08, Chic Lotz + keith Montgomery <kamchic@JPS.NET> wrote:
From: Chic Lotz + keith Montgomery <kamchic@JPS.NET>
Subject: ^6 Electric Shino
To: CLAYART@LSV.CERAMICS.ORG
Date: Tuesday, June 10, 2008, 4:31 PM
Have been looking for that ^6 Electric Shino recipe that combines a
White Satin and Nutmeg. I remember it was discussed quite a bit a
few years ago. Tried searching the archives, but it says I am not
authorized to do so. If you have the two recipes for mixing this
glaze, can you email them to me off line. I'd also like to know the
author of that glaze if possible......
Thanks, Chic Lotz
Chic@PotteryPoet.com
www.PotteryPoet.com
thepotter on wed 11 jun 08
> White Satin and Nutmeg.
Don't know if this is what you are looking for but this "white satin matt
and nutmet were in Ceramics Monthly Feb 03.
White Satin Matt Cone 6
Gerstley Borate 31.63
Talc 13.95
F-4 Feldspar 19.80
EPK 4.98
Silica 29.64
Zircopax 5.11
Bentonite 1.99
Nutmeg Cone 6
Dolomite 23.30
Spodumene 23.30
Frit 3134 6.80
OM4 Ball Clay 23.30
Silica 23.30
Red Iron Oxide 1.07
Yellow Ochre 3.24
Tin Ox 4.85
Bentonite 1.94
Good Luck.
Bev in RI getting ready for a studio show this weekend.
Can't decide if I have too many pots or not enough.....I guess we will find
out!
| |
|