Randy McCall on tue 5 aug 08
Has anyone used the Noxema Blue base to create a bright transparent green?
If you have would you let me know how it came out. Amout of copper carb you
used?
Randy
Cotton Patch Pottery
members.tripod.com/~McCallJ/index.html
Christine Campbell on wed 6 aug 08
Years ago, I printed out both recipes
when they were originally posted to
clayart.
I am NOT a glaze person, but they worked
well for me.
Mix thin to easily see outline
of fingernail.
THIN coats as it RUNS.
TRANSPARENT GREEN CONE 4-6
Custer Feldspar 38.1
Dolomite 10.0
EPK 9.6
Silica 9.5
Gerstley Borate 9.5
Zinc Oxide 9.4
Copper Carb 4.9
Chris Campbell - in North Carolina
--
Chris Campbell Pottery LLC
9417 Koupela Drive
Raleigh NC 27615-2233
Designs in Colored Porcelain
1-800-652-1008
Fax : 919-676-2062
website: www.ccpottery.com
wholesale : www.wholesalecrafts.com
| |
|