glaze test for randy's 3 in 1 ^6 ox. alisa version

updated wed 17 sep 08

 

Alisa Clausen on tue 16 sep 08


Recipe Name: Randy's 3 in 1 glaze Alisa version

Cone: 6 Color:
Firing: Oxidation Surface: Glossy

Amount Ingredient
5 Frit--Ferro 3134
41 Feldspar--Custer
12 Ball Clay--Old Mine #4
10 Red Art
10 Spodumene--Foote
6 Dolomite
10 Bone Ash
10 Silica
6

110 Total


Unity Oxide
.067 Li2O
.105 Na2O
.176 K2O
.133 MgO
.519 CaO
1.000 Total

.493 Al2O3
.057 B2O3
.025 Fe2O3

3.442 SiO2
.011 TiO2
.103 P2O5

7 Ratio
6.6 Exp

Comments: A gloss, to semi gloss gl aze with an overall warm beige color.
Milky where thickest. Smooth surface. I like this glaze the best of the 4
tests because of it's warmer color. However, sill no overlapping or
breaking effects, as glaze is quite evenloy covering.