glaze test for randy's 3 in 1 ^6 ox. tim's version resend and correction

updated wed 17 sep 08

 

Alisa Clausen on tue 16 sep 08


Recipe Name: Randy's 3 in one Tim version

Cone: 6 Color:
Firing: Oxidation Surface: Glossy

Amount Ingredient
47.1 Feldspar--Custer
15.5 Spodumene--Foote
19.9 Dolomite
9.8 Silica
7.3 Bone Ash
5.1 Gerstley Borate--1999
1.4 Kaolin--EPK

106 Total


Unity Oxide
.072 Li2O
.066 Na2O
.127 K2O
.251 MgO
.484 CaO
1.000 Total

.305 Al2O3
.045 B2O3
.008 Fe2O3

2.158 SiO2
0 TiO2
.053 P2O5

7.1 Ratio
7.3 Exp