search  current discussion  categories  glazes - cone 4-7 

coloratns for testing a base ^6 ox.

updated sun 28 sep 08

 

Alisa Clausen on fri 26 sep 08


Hi Clayart
Some have asked me for my list of color tests when I test a base I am
interested in.
These are the combinations I use: A lot, but I get to see a lot of results
when they are fired.

Consistent tests and a lot of work can get results!




Glaze test colorants for testing bases ^6 ox.



1. Base

2. 1 Co. Carb.

3. 3 Co. Carb

4. 1 Co. Carb. 2 Rutile

5. 1 Co. Carb. 4.5 Rutile (Lt. Stormy Blue)

6. 1 Co. Carb. 6 Rutile (Caribbean Sea Green)

7. 1 Co. Carb. 2 Chrome

8. 1 Co. Carb. 1 RIO

9. 1 Co. Carb. 3 RIO

10. 1 Co. Carb. 5 Ochre

11. 2 Co. Carb. 1 Tin

12. 3 Rutile

13. 6 Rutile (Bone)

14. 6 Rutile, 6 RIO (Raw Sienna)

15. 3 Cu. Carb.

16. 6 Cu. Carb.

17. 3 Cu. Carb., 3 Rutile

18. 1.5 Co. Carb. 3 Cu. Carb. 6 Rutile (Variegated Slate Blue)

19. 1 Co. Carb. 0.75 Cu. Carb, 6 Rutile, 3 RIO (Variegated
Blue)

20. 4 Cu. Carb. 4 Rutile (Spearmint)

21. 1 Co. Carb. 4 Rutile, 2 RIO (Floating Blue)

22. 1 Co. Carb. 6 Rutile, 0.5 RIO (Sky Blue)

23. 5 RIO

24. 10 RIO

25. 5 RIO, 5 Ochre

26. 5 Tin

27. 10 Tin

28. 5 Zircopax

29. 10 Zircopax

30. 5 Titanium

31. 10 Titanium

32. 5 Titanium, 5 RIO

33. 1.5 Titnaium, 15 RIO (Waxwing)

34. 1 Rutile, 12.5 RIO (Waterfall Brown)

35. 2 Co. Carb, 9 RIO (Licorice)

36. 4 Manganese Diox. 6 Rutile (Oatmeal)

37. 4 Manganese, 0.4 Co. Carb, 6 Rutile (Field Mouse)

jean szostek on sat 27 sep 08


hi alisa
i hav e a question for you : do you work 24/24 hours per day?
its fantastic the work you do for all of us
thanks again greatings jean
----- Original Message -----
From: "Alisa Clausen"
To:
Sent: Friday, September 26, 2008 9:01 PM
Subject: Coloratns for testing a base ^6 Ox.


> Hi Clayart
> Some have asked me for my list of color tests when I test a base I am
> interested in.
> These are the combinations I use: A lot, but I get to see a lot of
> results
> when they are fired.
>
> Consistent tests and a lot of work can get results!
>
>
>
>
> Glaze test colorants for testing bases ^6 ox.
>
>
>
> 1. Base
>
> 2. 1 Co. Carb.
>
> 3. 3 Co. Carb
>
> 4. 1 Co. Carb. 2 Rutile
>
> 5. 1 Co. Carb. 4.5 Rutile (Lt. Stormy Blue)
>
> 6. 1 Co. Carb. 6 Rutile (Caribbean Sea Green)
>
> 7. 1 Co. Carb. 2 Chrome
>
> 8. 1 Co. Carb. 1 RIO
>
> 9. 1 Co. Carb. 3 RIO
>
> 10. 1 Co. Carb. 5 Ochre
>
> 11. 2 Co. Carb. 1 Tin
>
> 12. 3 Rutile
>
> 13. 6 Rutile (Bone)
>
> 14. 6 Rutile, 6 RIO (Raw Sienna)
>
> 15. 3 Cu. Carb.
>
> 16. 6 Cu. Carb.
>
> 17. 3 Cu. Carb., 3 Rutile
>
> 18. 1.5 Co. Carb. 3 Cu. Carb. 6 Rutile (Variegated Slate
> Blue)
>
> 19. 1 Co. Carb. 0.75 Cu. Carb, 6 Rutile, 3 RIO (Variegated
> Blue)
>
> 20. 4 Cu. Carb. 4 Rutile (Spearmint)
>
> 21. 1 Co. Carb. 4 Rutile, 2 RIO (Floating Blue)
>
> 22. 1 Co. Carb. 6 Rutile, 0.5 RIO (Sky Blue)
>
> 23. 5 RIO
>
> 24. 10 RIO
>
> 25. 5 RIO, 5 Ochre
>
> 26. 5 Tin
>
> 27. 10 Tin
>
> 28. 5 Zircopax
>
> 29. 10 Zircopax
>
> 30. 5 Titanium
>
> 31. 10 Titanium
>
> 32. 5 Titanium, 5 RIO
>
> 33. 1.5 Titnaium, 15 RIO (Waxwing)
>
> 34. 1 Rutile, 12.5 RIO (Waterfall Brown)
>
> 35. 2 Co. Carb, 9 RIO (Licorice)
>
> 36. 4 Manganese Diox. 6 Rutile (Oatmeal)
>
> 37. 4 Manganese, 0.4 Co. Carb, 6 Rutile (Field Mouse)


--------------------------------------------------------------------------------