floatin blue

updated sun 28 sep 08

 

John Britt on fri 26 sep 08


Yes I use it and it is really nice in cone 6 reduction :

FLOATING BLUE Cone 6
Nepheline Syenite 47.30
Gerstley Borate 27.00
Silica 20.30
EPK Kaolin 5.40

Rutile 4.00
Red Iron Oxide 2.00
Cobalt Oxide 1.00


This glaze is also great!

GNU BLUE Cone 6
Alberta Slip 75.00
Gerstley Borate (Gillispie Borate) 15.00
Dolomite 5.00
Silica 4.00

Rutile 4.00

Hope it helps,


John Britt
www.johnbrittpottery.com/wks.htm

jean szostek on sat 27 sep 08


thank you john
im going to try it out, and surtenly the second, is this a rutile blue?
thanks greatings jean
----- Original Message -----
From: "John Britt"
To:
Sent: Saturday, September 27, 2008 2:51 AM
Subject: Re: Floatin Blue


Yes I use it and it is really nice in cone 6 reduction :

FLOATING BLUE Cone 6
Nepheline Syenite 47.30
Gerstley Borate 27.00
Silica 20.30
EPK Kaolin 5.40

Rutile 4.00
Red Iron Oxide 2.00
Cobalt Oxide 1.00


This glaze is also great!

GNU BLUE Cone 6
Alberta Slip 75.00
Gerstley Borate (Gillispie Borate) 15.00
Dolomite 5.00
Silica 4.00

Rutile 4.00

Hope it helps,


John Britt